徐建伦
,
宋波
,
陈继开
,
韩其勇
,
蒋国昌
金属学报
用气液平衡法,在密封Mo反应室中研究了1873K下Fe液中Bi蒸气溶解平衡及第三组元Ni,Mn对其的影响,测定了1873K下Bi在Fe液中的溶解量(wt—%)为0.16。Ni,Mn增加Bi的溶解量,其活度相互作用系数为e_(Bi)~(Ni)=-0.20,e_(Bi)~(Mn)=-0.19。
关键词:
Bi
,
liquid Fe
,
dissolution equilibrium
,
interaction coefficient
ZHANG Xiaodong HAN Qiyong University of Science and Technology Beijing
,
Beijing
,
ChinaCHEN Dong Hebei Institute of Metallurgy
,
Shijiazhuang
,
China HAN Qiyong Professor
,
Dept.of Physics and Chemistry
,
University of Science and Technology Beijing
,
Beijing 100083
,
China
金属学报(英文版)
The dissolution equilibrium of magnesium vapour in liguid Fe has been studied in a two-tem- perature-zone furnace at 1600℃ by use of the vapour pressure method.The equilibrium con- stant for the reaction Mg_((g))=[Mg]and the free energy of solution obtained are: K=a_(Mg)/P_(Mg)=0.0236 ΔG°(wt-%)=58300 J/mol
关键词:
liquid Fe
,
null
,
null