The origin of low ductility at elevated tempera- ture in the cryogenic and non-magnetic steel Fe-23Mn-4Al-5Cr-0.3C was investigated by means of impact test at elevated temperatures,opti- cal microscope,SEM and TEM.The experimental results indicate that the impact toughness lowers with increasing testing temperature,and exhibits a low trough of ductility from 865℃ to 1050℃ and a peak value at 1150℃.The intergranular fracture occurs in the temperature region of low ductility and the transgranular ductile rupture below this re- gion principally.There is a process of precipitating, gathering,growing,and dissolution of carbide (FeMnCr)_(23)C_6 and AlN between 500℃ and 1000℃.The coalescence of microvoids caused by the process at grain boundaries results in the intergranular fracture and the low ductility at ele- vated temperatures.