研究了在异丙醇-硝酸体系中单次分子镀流程制备Sm和Eu厚靶的实验条件.确定了在20 μm铍箔上进行Sm和Eu分子镀实验的最佳工艺条件为:两极间距3 cm,电流密度3.8 mA/cm2,分子镀过程持续1 h.用分光光度法测定了分子镀的沉积效率均高于95%,所制备Sm和Eu靶膜的厚度分别在1.6和1.5 mg/cm2.