采用化学共沉淀法成功地制备出适用于彩电显象管内荧光体着色的CoxR1-xAl2O4(R=Zn、 Mg, x=0.8~1.0)钴蓝颜料: 450nm波长处反射率最大提高18.2%, 600nm处反射率最大降低5%。通过对该颜料反射率的影响因素,如掺杂离子类型、掺杂浓度和Co2+离子浓度的探讨,结论如下:Zn2+、Mg2+改变钴蓝颜料反射性能的作用机理为晶格畸变引起Co2+3d轨道电子能级分裂程度的变化;对于掺杂离子Zn2+、Mg2+,x下限值分别约为0.85和0.8.
A kind of CoxR1-xAl2O4(R=Zn、Mg,x=0.8\sim1.0)cobalt blue pigment suitable for luminophor of color televisions was synthesized successfully by
using the chemical coprecipitation method. Compared with CoAl2O4 reflectivity, the increase of reflectivity of CoxR1-xAl2O4 is 18.2% at 450nm
and --5% at 600nm respectively. Through discussing some affecting factors on this kind of pigment such as doping cation type, doping content and Co2+
content, a conclusion can be drawn that the mechanism of reflectivity properties alteration of complex cobalt blue pigments caused by doping cations Zn2+,
Mg2+ is Co2+3d electronic energy level cleavage due to lattice distortion. The lower limit value of x of Zn2+, Mg2+ is 0.85 and 0.8 respectively.
参考文献
[1] | |
[2] | Kingery W D, 等. 陶瓷导论. 北京:中国建筑工业出版社,1982. 62--63. [2] Weast R C. Handbook of Chemistry and Physics, 70th.Edition. Boca, Florida, U.S.A:CRC Pr.,Inc.,1989--1990. [3] Wold A, Dwight K. In: Solid State Chemistry: Synthesis, Structure, and Properties of Selected Oxides and Sulfides, New York:CHAPMAN & |