This paper describes a way to improve the weld quality through suppressing the porosity formation and restraining the growth of columnar grains by using a weaving beam in laser welding. The experimental results show that the N2 porosity of beam-weaving laser welding low carbon steel can be remarkably reduced with increasing weaving frequency, and porosity can be eliminated when the weaving amplitude is only 0.5 mm; and the Ar porosity in the weld metal is decreased with increasing weaving frequency and amplitude when the welding speed is higher than 0.5 m/min. The beam-weaving laser welding of ultra-fine grained steel has been investigated. The experimental results show that beam-weaving laser welding with appropriate amplitude and frequency can partly restrain the growth of the columnar grain and improve the tensile strength of the weld metal.