为了提高Al2O3-MgO-ZrO2层状复合陶瓷烧嘴材料的强度、韧性和热震性能,制备了SiC/SiO2-Al2 O3-MgO-ZrO2新型陶瓷材料.结果表明,SiC/SiO2复合纳米粉体的添加大大增加了材料的体积密度,增强了材料的抗弯强度和断裂韧性.特别是经1850℃焙烧的样品,当SiC/SiO2复合纳米粉体的含量为7%(质量分数)时,试样的抗弯强度和断裂韧性分别提高了23.1%和25.5%,在热震温差超过1000℃的恶劣条件下,其残余抗弯强度保持率仍高达69%.SEM观察表明,单纯的Al2O3-MgO-ZrO2材料的断面有游离的柱状颗粒存在,而添加SiC/SiO2的样品,不同氧化物和非氧化物颗粒紧密结合,形成光滑圆润的波浪状结构,这一显微结构对提高材料的力学性能有重要作用.

参考文献

[1] Merzhanov A G .Combustion processes that synthesize materials[J].J Mater Process Techn,1996,56:222.
[2] Deng J X;Zheng Z C;Ding Z L et al.Erosion wear of ceramic and cemented carbide nozzles in dry sand blasting process[J].British Ceram Trans,2003,102(02):61.
[3] 冯益华,邓建新.B4C/(W,Ti)C陶瓷喷砂嘴冲蚀磨损机理研究[J].摩擦学学报,2004(04):346-350.
[4] 员冬玲 .层状复合陶瓷喷嘴的设计制造及其应用研究[D].山东大学,2009.
[5] Wakuda M;Yamauchi Y;Kanzaki S .Effect of workpiece properties on machinability in abrasive jet machining of ceramic materials[J].Precision Engineering,2002,26(02):193.
[6] Wakuda M;Yamauchi Y;Kanzaki S .Material response to particle impact during abrasive jet machining of alumina ceramics[J].J Mater Process Techn,2003,132(1-3):177.
[7] 孙军龙 .新型B4C基复合陶瓷喷嘴研究开发[D].济南:山东大学,2007.
[8] Hanadi Ghanem;Helmut Gerhard;Nadejda Popovska .Paper derived SiC-Si_3N_4 ceramics for high temperature applications[J].CERAMICS INTERNATIONAL,2009(3):1021-1026.
[9] Luo fa;Zhu dongmei;Su xiaolei;Zhou wancheng .Properties of hot-pressed of SiC/Si3N4 nanocomposites[J].Materials Science & Engineering, A. Structural Materials: Properties, Misrostructure and Processing,2007(1-2):7-10.
[10] 马玉柱 .ZrO<,2>/Al<,2>O<,3>系层状复合陶瓷材料的研究[D].重庆大学,2002.
[11] A. Rittidech;L. Portia;T. Bongkarn .The relationship between microstructure and mechanical properties of Al_2O_3-MgO ceramics[J].Materials Science & Engineering, A. Structural Materials: Properties, Misrostructure and Processing,2006(0):395-398.
[12] Zhang, P.;Hui, W.;Zhang, Y.;Ren, X.;Zhang, D. .Molecular dynamics simulation for the rapid solidification process of MgO-Al _2O _3-SiO _2 glass-ceramics[J].Journal of Non-Crystalline Solids: A Journal Devoted to Oxide, Halide, Chalcogenide and Metallic Glasses, Amorphous Semiconductors, Non-Crystalline Films, Glass-Ceramics and Glassy Composites,2012(12/13):1465-1473.
[13] Qing-song Ma;Yan Ma;Zhao-hui Chen .Fabrication and characterization of nanoporous SiO_2 ceramics via pyrolysis of silicone resin filled with nanometer SiO_2 powders[J].CERAMICS INTERNATIONAL,2010(8):2269-2272.
[14] Soumya Shankar Ghosh;Pijush Kanti Mandal;Rabindranath Majumdar .Replication of jute stem for porous cellular ceramics/composites in the SiO_2–SiC–C System[J].CERAMICS INTERNATIONAL,2010(7):2063-2071.
[15] Gomez E;Echeberria J;hurriza I et al.Liquid phase sintering of SiC with additions of Y2O3,Al2O3 and SiO2[J].Journal of the European Ceramic Society,2004,24(09):2895.
[16] Li L;Wu X;Zhu Z .Microwave dielectric materials based on the MgO-SiO2-TiO2 system[J].Journal of the European Ceramic Society,2003,23(14):2569.
[17] Ohji T.;Choa YH.;Niihara K.;Jeong YK. .Strengthening and toughening mechanisms of ceramic nanocomposites[J].Journal of the American Ceramic Society,1998(6):1453-1460.