高级检索

通过对发生脆性断裂的钛合金TB5试制板坯的化学成分、断口形貌、微观组织进行分析,结果表明板坯化学成分均匀,满足国标要求;断口呈解理及准解理断裂特征,断口有析出相存在,但无夹杂物出现;板坯组织为粗大的等轴晶,晶内有长针片状的析出相,分布均匀且规则.分析显示:板坯发生脆断行为与化学成分无关,导致板坯脆性断裂的原因是板坯晶粒粗大,同时晶粒内析出了粗大的析出相,割裂了β基体,阻碍变形时位错运动,严重降低了板坯的塑性.

参考文献

[1] Hirowo G SUZUKI;Hideki FUJII .Deformation characteristics of Ti-15V-3Cr-3Sn-3Al at elevated temperature[J].ISIJ International,1991,31(08):814-819.
[2] 张喜燕;赵永庆;白晨光.钛合金及应用[M].北京:化学工业出版社,2004:92.
[3] Temhiko INABA;Kei AMEYAMA;Masaharo TOLIZANE .Formation of(α+β)micmdulea strocture in a Ti-15V-3Cr-3Sn-3Al alloy[J].ISIJ International,1991,31(08):792-798.
[4] Ohyama H;Miyamoto A;Aahida Y et al.Improvement of mict+ostructuie and tensile properties by wane working[J].Current Advancements in Molecular Medicines,1990,3(05):1592-1595.
[5] Morinaga M;Yukawa N;Maya T.The 6th world conference on titanium[A].France:Paris,1989:1601.
[6] Niinomi M;Kobayashi T;Inagaki I et al.The effect of defonmation-induced transformation on the fracture toughness of commeroial titanium alloys[J].Metallurgical and Materials Transactions A:Physical Metallurgy and Materials Science,1990,21(06):1733-1744.